TBA - NAVSEA TECHNICAL PUBLICATION

S9074-AR-GIB-010/278

TABLE XVIII. RT acceptance criteria for steel (carbon. allov. and corrosion resistant). titanium. and titanium alloy castings. - Continued

Maximum severity level

ASTM standard 2

Thickness (inches)

Criticality Level 1

Hot tear, crack

Insert. chaplet

Shrinkage Porosity Inclusion

CA 3 CB 3 CC 3

E 186

1

A 3

B 3

None None

CA 4 CB 4 CC 4

2

E 186

EA 3, EB 3

None

A 4

B 4

Over 2 to 4-1/2

CA 5 CB 5 CC 5 CA 2 CB 2 CC 2 CA 3 CB 3 CC 3

3

EA 4, EB 4

E 186

None

B 5

A 5

1

E 280

B 3

A 3

None

None

Over 4-1/2

2

E 280

None

EA 3, EB 3

B 4

A 4

CA 5 CB 5 CC 5

A 5

B 5

EA 4, EB 4

None

E 280

3

Criticality level 1: Areas requiring 75 percent minimum RT coverage see (12.5.3). Criticality level 2 : Areas requiring 50 percent minimum RT coverage see (12.5.3). Criticality level 3 : Areas not requiring RT but are inadvertently radiographed for informartion purposes. 1.

2.

Evaluation or radiographs for acceptance shall be in accordance with the applicable ASTM stanbard. ASTM E 186 shall be used for evaluation purposes.

3.

Original 115