6. Place the subsequent layers of glass fibre onto the matrix and thoroughly wet out the glass fibre with matrix. 7. Exercise 6 - Curing 1. Apply peel ply on top of the glass fibre and remove the air.

2.

Apply release film onto the peel ply.

3.

Place the thermocouple onto the release film.

4.

Apply breather fabric onto the release film.

5. Insert a vacuum hose and cover the entire panel with vacuum foil. Ensure that the vacuum foil is sealed to the vacuum tape all the way around.

6.

Apply vacuum to the panel, check for air leaks, and fix air leaks.

7. Place a heating blanket onto the panel and adjust the temperature to the curing temperature in the TDS. Note the time that the blanket reaches the curing temperature.