Coatings 2026 , 16 , 299
12of 25
Optical surface profilometry provides a much more comprehensive and detailed characterisation of the structure of the coated samples than is possible with Bendtsen surface roughness measurements. Given that Bendtsen surface roughness and optical profilometry use different measurement techniques, the results obtained from these two methods may not always correspond exactly. Optical surface profilometry images (contour images) for BASE, A6, B6, MB6, RSB1 and RDB2 are shown in Figure 2. The long-range waviness is distinctly observable. However, differences in surface roughness could not be observed directly from Figure 2. To draw conclusions about surface roughness, the surface profiler datasets were processed using computer-aided calculations to obtain the filtered average roughness (Sa). Table 5 shows the unfiltered Sa; the short wavelength pass-filtered Sa; and Sc, Sv, and V s . Table5. Roughness parameters obtained from analyses of surface profiler images. Sa filtered indicates the average roughness after the elimination of waviness (wavelength cutoff 1 mm). The error limits indicate standard deviation.
Sa Unfiltered ( μ m)
Sa Filtered ( μ m) 4.4 ± 0.2 3.3 ± 0.0 3.0 ± 0.2 3.5 ± 0.1 3.2 ± 0.3 3.0 ± 0.1 4.8 ± 0.3 5.1 ± 0.3 4.6 ± 0.2 4.1 ± 0.4 4.1 ± 0.2
Sc (cm 3 m − 2 )
Sv (cm 3 m − 2 )
V s (cm 3 m − 2 )
Sample Name
Sc/Sv
Base paperboard 10.1 ± 0.6 Series A—IR 20%
BASE
6.7 ± 0.4 5.9 ± 1.2 6.1 ± 1.5 6.0 ± 0.7 6.4 ± 1.0 5.0 ± 0.5 7.6 ± 2.0 7.3 ± 0.9 6.4 ± 0.3 5.7 ± 0.6 6.6 ± 1.1
0.9 ± 0.1 0.8 ± 0.1 1.0 ± 0.3 0.9 ± 0.0 0.9 ± 0.1 0.8 ± 0.1 1.0 ± 0.1 1.0 ± 0.0 1.0 ± 0.1 0.9 ± 0.1 0.9 ± 0.1
11.1 ± 0.9 10.3 ± 0.7 8.5 ± 1.0 9.9 ± 0.7 11.0 ± 0.8 9.6 ± 0.8 12.0 ± 3.8 11.0 ± 1.3 9.5 ± 0.6 9.7 ± 0.7
11.0 ± 0.6 9.3 ± 1.3 9.5 ± 1.9 9.7 ± 1.0 10.5 ± 1.6 8.1 ± 0.8 12.8 ± 4.4 12.0 ± 1.7 10.2 ± 0.3 9.2 ± 1.0
A5 A6
8.4 ± 1.2 8.4 ± 1.6 8.8 ± 1.0 9.6 ± 1.5 7.3 ± 0.6 11.8 ± 4.4 11.0 ± 1.6 9.3 ± 0.3 8.4 ± 0.9 9.9 ± 2.1
Series B—IR 40%
B5 B6
Modified Series B—IR 40%—half of the IR frames are active
MB6
Reference thick single coating
RSA1 RSB1
Reference thick double coating
RDA1 RDA2 RDB2
11.2 ± 1.9 10.8 ± 2.1 Table 5 shows no significant differences in unfiltered Sa between BASE and the coated paperboards, indicating that all samples—whether metered with the soft-tip element or with the rod—exhibited a contour-type coating. A uniform coating layer is essential for achieving low gas transmission. The experimental scatter in unfiltered Sa was anticipated to be high due to the large-scale waviness in Figure 2 relative to the limited the image size. The filtered Sa values are shown in Table 5. The filtered Sa values show roughness values without the influence of waviness. As expected, the experimental scatter of the filtered Sa values was considerably lower than that of the unfiltered Sa values. The filtered Sa showed that the roughness of the multilayered samples exhibited substantially lower roughness than the uncoated paperboard. The samples with six thin layers without any pinholes (A6 and MB6) displayed the lowest surface roughness. The diameter of cellulose fibres (approximately 30 μ m for softwood) falls within the length scale of roughness (0–1000 μ m). This implies that the reduced filtered Sa observed for thin multilayer coatings likely reflects a high degree of fibre coverage and filling of surface voids between cellulose fibres.
https://doi.org/10.3390/coatings16030299