PAPERmaking! Vol12 Nr2 2026

Coatings 2026 , 16 , 299

5of 25

2. Materials and Methods 2.1. Materials

Hydroxypropylated and oxidised potato starch (Solcoat P 55) was supplied by Solam GmbH, Emlichheim, Germany. Its Brookfield viscosity (100 rpm) at 25% aqueous solution and50 ◦ C was about 82 mPas, according to the manufacturer. Hydroxypropylated starches are widely used as food additives [75]. Poly(ethylene glycol), PEG (Carbowax Sentry PEG 600) was purchased from Univar Sweden AB, Malmö, Sweden. According to the supplier, the average molecular weight range and density at 20 ◦ C were 570 to 630 and 1.126gcm − 3 , respectively. The PEG used has approval as a component of articles intended for contact with food (FDA 21 CFR 178.3750). Bentonite, Cloisite Na + , was purchased as a powder from Southern Clay Products, Gonzales, TX, USA. The aspect ratio of the bentonite layers was 75–100 nm [63]. The used bentonite powder contained 7.5% water (by wt.), as analysed gravimetrically. Bentonite is authorised as an additive for plastic materials in contact with foods with no specific restrictions (Commission Regulation (EU) No 10/2011). Sodium hydroxide was used for pH adjustments. All chemicals were used without further purification. The used substrate was an uncoated triple-ply paperboard with a bleached top layer from Billerud AB, Frövi, Sweden. The board had a grammage of 270 g m − 2 and a thick- ness of 390 μ m. The water absorptiveness on the brown unbleached side measured 23.3 ± 0.8gm − 2 , according to Cobb60 tests (ISO 535:1991). 2.2. Methods 2.2.1. Preparation of Barrier Dispersion The barrier dispersion (coating colour) was based on the starch/bentonite/PEG for- mulations described by Olsson et al. [74], with two principal deviations: citric acid was omitted and a higher-molecular-weight plasticizer, PEG 600, was used instead of the PEG 400 that was applied in the earlier work [74]. The as-received starch was gelatinised under vigorous stirring at 95 ◦ C for 45 min. The resulting solid content of the aqueous starch solution was 26%. The as-received PEG was heated to above 50 ◦ C to ensure a liquid state and added to the hot starch solution about 10 min after the preparation of the starch solution was completed. A Cowles-type impeller was used for the dispersion of bentonite. The dispersion took place by adding bentonite to water under high stirring. Stirring continued for about 30 min after the last amount of bentonite powder had been added. The resulting solid content of the bentonite dispersion was 8.5%. This corresponded approximately to the maximum dry solid content that can be achieved for a manageable bentonite suspension of the type used. The bentonite suspension was then pumped into the tank that contained the starch/PEG solution. Studies indicate that bentonite clay is intercalated but not delaminated in this type of dispersion [61]. To slightly increase the bentonite content of the final barrier dispersion, a small amount of dry bentonite powder was added to the bentonite/starch/PEG suspension. Following this addition of bentonite powder, the barrier dispersion was stirred for 30 min and adjusted to pH = 8.5. The composition of the final barrier dispersion formulation is presented in Table 1. The final coating colour was then pumped into the machine tank. The dry solid content and the viscosity of the final barrier dispersion used in all coating trials were 19.5% and 0.90 Pas (Brookfield 100 rpm at 32 ◦ C), respectively. The temperature of the coating colour during the pilot trials was 32 ◦ C.

https://doi.org/10.3390/coatings16030299

Made with FlippingBook Online newsletter maker