Coatings 2026 , 16 , 299
8of 25
unwinding position in the front of the pilot machine for application of the next layer. The total coat weight after 6 thin layers was about 5 g m − 2 . The coat weight of each individual layer ranged from 0.45 to 1.5 g m − 2 , with the highest coat weights obtained during the first coating passes. Drying between successive layers was applied to the double-coated reference samples as well. The paperboards entering the coater for MA2, MB6, RDA2 and RDB2 were A1, B5, RDA1 and RDB1, respectively. The coat weights were calculated from the measured consumption of barrier dispersion. The coat weights and drying conditions are summarised in Table 2. The drying units utilised for the reference samples, i.e., the thick single- and double- coatings with coat weights of each individual layer >3 g m − 2 , operated at higher power relative to those employed for the thin multilayer samples (see Table 2).
2.2.3. Analyses of Coated Paperboard Pinholes
Pinholes were quantified in accordance with SS-EN 13676. A colouring solution prepared by dissolving 0.5 g of dyestuff, Crocein Scarlet MOO (CAS 5413-75-2), in 100 mL of ethanol, was used. The coated side of each specimen was exposed to the solution for 5 min, after which the surplus was removed, and any coloured spots were counted. The results were expressed as the number of pinholes/dm 2 , with an upper detection limit of 30 pinholes/dm 2 . All experiments were performed within one week after the coating trials. For the pinhole measurements and all other analyses mentioned below, the samples were stored at 23 ◦ C and 50% relative humidity (RH) prior to measurement. The results from the pinhole measurements were performed in five replicates. Surface Structure—Air Flow Method A Bendtsen apparatus (Bendtsen Tester, Model 58-27, Messmer Buchel, The Nether- lands) was used to test surface roughness according to ISO 8791-2. This method is based on air flow, and the test pressure was 1.47 kPa. All measurements were repeated 21 times, except for those for the uncoated paperboard, which were repeated 42 times. The measure- ments on the uncoated cardboard were performed on the unbleached brown side. Profilometry—Images, Roughness and Void Volume An optical surface profiler (ContourGT-K, Bruker Nano Inc., Tucson, AZ, USA) operated in VSI mode along with the Vision 64 software (Bruker Nano Inc., Tucson, AZ, USA) was used to acquire contour images and determine roughness parameters listed in Table 3. All measurements were performed in triplicate, except for those for the uncoated paperboard, which were repeated 10 times. The measurements employed a Michelson 5 × objective with an optical resolution of 2.2 μ mand a 0.55 × field-of-view lens. The pixel size of all images was 3.5 μ m. Stitched images (rectangular stitch; 10 mm × 10mm) were used for all roughness calculations. The stitched raw images were optimised by applying a 3-pixel median statistic filter, followed by data restoration (data interpolation from valid pixels around eventual missing pixels) and finally by gentle tilt removal (plane fit). The natural and positive volumes were carefully controlled such that the natural volume equalled the negative volume and that the positive volume equalled 0nm 3 after the removal of any tilt impact. The optimised images were then used in the analysis of the roughness parameters.
https://doi.org/10.3390/coatings16030299
Made with FlippingBook Online newsletter maker