Coatings 2026 , 16 , 299
10of 25
330 mL and the oxygen volume ( V oxygen ) was recorded as a function of time ( t ). Before each experiment, the sample cell was flushed with nitrogen to reduce the oxygen concentration to approximately 1% (by vol.). The temperature and RH were maintained at 23 ◦ Cand 50%, respectively. Further experimental details are provided elsewhere [78]. The AOIR, defined as ( dV oxygen dt ), was calculated from the initial linear part of the curve V oxygen vs. t , under conditions where the oxygen pressure inside of the cell is small in comparison with the oxygen pressure outside of the cell. dV oxygen dt lin = (2) where p atm is the atmospheric pressure, p i is the oxygen pressure in the cell measured at the initial time t i , and p f is the oxygen pressure in the cell measured at the final time t f , according to Larsen et al. [79]. Experimental points up to an oxygen concentration of 4 ± 1% (by vol.) oxygen were used for the linear curve fit of the initial part of the curve V oxygen vs. t . However, experimental points at higher oxygen concentration were also included for samples BASE, A1, RSB1 and RDB1 due to the rapid increases in oxygen concentration. All AOIR measurements were completed within three months after the coating trials and conducted in duplicates. V cell p f − p i p atm t f − t i
3. Results 3.1. Pinholes and Surface Structure
The quantification of pinholes in the coated sheets was conducted as an initial assess- ment of their barrier properties. Surface roughness was evaluated using both the Bendtsen air leakage method and surface profilometry, supplemented by V s measurements. This approach offers valuable insights into the interfacial interactions between the coating dis- persion and the substrate. The present study further examined the substrate’s responses to applied forces during application and metering, as well as its interaction with the aqueous phase throughout the interval between application and immobilisation. Table 4 displays the number of pinholes and the Bendtsen surface roughness values for the samples analysed in this study. The multilayer approach in combination with the selected coater and metering device was used to achieve coated paperboard free of pinholes even at low coat weights. The multilayered samples A5, A6 and MB6 contained no pinholes, indicating that a uniform and continuous coating had been achieved. In contrast, the single- and double-coated reference samples exhibited significantly higher numbers of pinholes. This occurred notwithstanding the fact that certain reference samples exhibited a higher coat weight compared with any of the multilayer-coated paperboards. Notably, for the multilayer coatings, the incidence of pinholes could not be predicted based on Bendtsen roughness measurements. Instead, drying conditions—particularly the IR drying settings—appear to be the decisive factor governing pinhole formation. Raising the IR power from 20% to 40% resulted in more pinholes (cf. Series A and Series B in Table 4), indicating that the 40% IR setting caused premature film formation. This effect is further supported by a comparison between A2 and MA2, which exhibited 19.0 pinholes/dm 2 and a pinhole density beyond the measurable range, respectively. The only difference between these two samples was the higher IR power for MA2. Excessively intense IR drying of the multilayered samples, as in the Modified Series A samples, resulted in severe blistering, which became evident in the third layer.
https://doi.org/10.3390/coatings16030299
Made with FlippingBook Online newsletter maker