PAPERmaking! Vol12 Nr2 2026

PAPER making! FROM THE PUBLISHERS OF PAPER TECHNOLOGY INTERNATIONAL ® Volume 12, Number 2, 2026

requires low-molecular-weight C-PAM, which has shorter chain lengths but is present in greater numbers. In mixed- filler systems (talc:GCC = 50:50), higher proportions of 8 × 10 6 C- PAM increased talc retention, while higher proportions of 6 × 10 6 C-PAM enhanced GCC retention. Results indicate that high-molecular weight C-PAM is more effective for large suspended solids, whereas lower-molecular weight C-PAM better retains smaller fillers under limited polymer dosage. These findings provide practical guidelines for selecting retention aid molecular weight based on filler particle size in papermaking. MOULDED PULP “ PFAS-free molded pulp trays: effects of pulp type, refining level, and cellulose nanofibrils or biowax addition on tray performance ” , Jinwu Wang, Seongkyung Park & Colleen C. Walker, Cellulose , Vol.33, 4077 – 4104 (2026). Polyfluoroalkyl substances (PFAS) have been widely used in food packaging due to their thermal and liquid resistance; however, health and environmental concerns have driven efforts to develop safer alternatives. This study investigates the production of PFAS-free molded pulp trays using a pilot-scale fiber molding system scalable for industrial applications. The process involves vacuum-assisted fiber deposition, membrane prepress dewatering, and hot pressing. Process parameters were first optimized using a formulation of bleached hardwood kraft pulp, bio-based wax, alkyl ketene dimer, and retention aids. This commercial formulation significantly reduced water and oil absorption of the trays as compared with those without bio-wax addition. Subsequently, the effects of pulp type, refining level, and cellulose nanofibril (CNF) addition on tray properties were evaluated under the optimal set of processing parameters, including pre-pressing (10kN, 18s) and hot-pressing (17kN, 220°C, 16s), whereas suction time was optimized based on pulp freeness to achieve the targeted weight of trays. Softwood pulps outperformed hardwoods in mechanical and barrier properties, requiring less refining and offering a more energy-efficient path to performative molded fiber. Unbleached softwood pulp demonstrated superior performance under the tested conditions. Unrefined hardwood pulp showed the lowest performance in mechanical and barrier properties, making it the most suitable candidate for refining or reinforcement by CNFs. Preliminary energy analysis showed direct refining was more efficient than CNF reinforcement. Findings provide design and material insights for scalable, PFAS-free production of molded fiber trays. “ Upcycling of industrial hemp byproducts into a sustainable molded fiber packaging system ” , Young-Ju Eun, Su Jung Hong & Young-Teck Kim, International Journal of Biological Macromolecules , Vol.361, May 2026, 151959. This study presents the fabrication and characterization of fully bio-based molded fiber composites using industrial hemp (Cannabis sativa L.) hurds, starch, and cellulose nanofibrils (CNF) for sustainable single-use packaging applications. Hemp hurds, a low-value agricultural byproduct, were directly upcycled into value-added molded fiber composites by varying their loadings to evaluate their influence on rheological, mechanical, and morphological properties. Rheological analysis revealed that excessive solid content increased slurry heterogeneity and entrapped microbubbles, reducing both storage and loss moduli. However, during hot pressing, these trapped air voids were released, resulting in densified fiber networks. Consequently, the mechanical performance improved with increasing hurd content up to a threshold. Among all formulations, the composite containing 20g of hemp hurds (H20) exhibited the most balanced properties, achieving high compressive (8.70 ± 0.34MPa), flexural (7.56 ± 0.51MPa), and impact strength (13.83 ± 1.19J/m), comparable to or exceeding those of the higher-loading formulation containing 28g of hemp hurds (H28). Compressive strength increased by more than 300% compared with conventional molded pulp reported in the literature, while flexural strength nearly doubled ( ∼ 90% increase) from

Page 6 of 13

Technical Abstracts

Made with FlippingBook Online newsletter maker