PAPERmaking! Vol12 Nr2 2026

Coatings 2026 , 16 , 299

15of 25

3.2. Grease Resistance and Oxygen Barrier Properties Analyses of grease resistance and oxygen transmission were carried out for a selected subset of samples. The AOIR, OTR and Kit ranking numbers are shown in Table 7. The variation in AOIR values for Series A aligns well with the corresponding decrease in pinhole surface density (cf. Table 4). A marked reduction in the AOIR—to values around 10mL day − 1 —was observed from three layers onwards. Due to experimental scatter, distinguishing between the AOIR values for the four samples in Series A with three to six layers was not possible. The higher IR power in Series B compared with that in Series A resulted in higher AOIR values, consistent with the increased pinhole densities for Series B. Turning off the IR radiation on one side of the web for the sixth layer in Series B gave a significantly lower AOIR (cf. M6 and MB6), demonstrating that defects can be reduced by lowering the total IR power. All reference samples (RSB1, RDB1 and RDB2) possessed an AOIR rather similar to that observed for A1 (one thin layer). Table 7 clearly shows that thin multilayer coatings provide lower oxygen transmission than one or two thick coating layers. Table 7 also includes the OTR for A6 and RDB1, measured according to the ASTM D 3985-05 standard. All other samples without pinholes (see Table 4) are likely to exhibit OTRs in the same range as A6. Even if a substantial decrease in the AOIR with an increasing number or layers in Series A was observed, the OTR was still too high to be regarded as a sufficient oxygen barrier for sensitive food packaging applications [83]. The OTR values presented in Table 7 should be compared with the oxygen barrier properties of films produced by laboratory-scale casting. Zeppa et al. [68] reported that the oxygen permeability of starch– montmorillonite cast films ranges from 66 to 239 cm 3 · μ m · m − 2 · day − 1 (pure oxygen was used as the permeant), depending on the type of plasticiser and montmorillonite employed. Based on the densities of the individual dry components, the density of the dry coating layers used in the present work can be approximated as 1.58 g cm 3 . This corresponds to an average coating thickness of 3.2 μ m for A6. The OTR value measured for A6 shown in Table 7 is higher than would be expected from the permeability values for cast free-standing films given by Zeppa et al. [68].

Table 7. AOIR, OTR and Kit rating number for some of the samples presented in Table 2. The upper detection limit for OTR measurements was 1000 cm 3 m − 2 day − 1 atm − 1 . The error limits indicate range.

AOIR (mLday − 1 )

OTR (cm 3 m − 2 day − 1 atm − 1 )

Sample Name

Kit Rating Number

Base paperboard

BASE

663 ± 15 337 ± 44 43 ± 2 13 ± 9 6 ± 2 9 ± 4 11 ± 2

Series A—IR 20%

A1 A2 A3 A4 A5 A6

5

12 12

511 ± 267

Series B—IR 40%

B6

23 ± 6

8

Modified Series B—IR 40%—half of the IR frames are active

MB6

7 ± 1

12

Reference thick single coating >1000 Reference thick double coating

RSB1

254 ± 38 253 ± 30 135 ± 9

RDB1 RDB2

https://doi.org/10.3390/coatings16030299

Made with FlippingBook Online newsletter maker