Coatings 2026 , 16 , 299
19of 25
dried using gentle IR power) exhibited fewer pinholes than any of the thick double-coated samples. This clearly highlights the benefits of thin multilayered coatings in combination with optimised drying conditions. In the IR drying of barrier-coated paper and paperboard, Heilmann [48] emphasised the importance of heating the initial sedimentation layer, noting that coatings should be dried from bottom to top to prevent premature film formation at the surface and penetration of the coating into the substrate. Premature film formation at the surface may in turn cause the formation of micro-blisters and pinholes. The reduced pinhole density observed in multilayered samples at 20% IR power (Table 4) indicates that thin individual layers enable sufficient heating of the substrate beneath the coating, thereby minimising defect formation. In contrast, drying at 40% IR power resulted in a markedly higher incidence of pinholes, indicating that too high IR power led to premature film formation of the uppermost part of the coating layer. A comparison between Series A and Modified Series A (Table 4) further demonstrated that overly intense IR drying of multilayered samples can induce pronounced blistering. This is most likely attributed to premature film formation resulting from elevated IR energy input relative to the enthalpy of vaporisation. At optimal conditions, the cooling effect of evaporation is expected to contribute to a temperature profile that promotes drying of the wet layer from bottom to top, as proposed by Heilmann [48]. The IR setup in MB6 resulted in coated sheets free from detectable pinholes (Table 4) and a relatively low AOIR (Table 7). The power setting of each active individual IR frame was 40% and 20% for the MB6 and Series A samples, respectively, with the total IR power kept constant. The higher power of each active IR frame for MB6—and thus the slightly shorter peak wavelength and greater penetration depth—may have promoted bottom-to-top drying, while the total IR power was low enough to prevent premature film formation. It is plausible that implementing a comparable drying strategy from the initial coating layer, deactivating all IR frames on the uncoated side, would have been successful in reducing both oxygen transmission and the pinhole density. A comparison between Tables 4 and 7 reveals that the oxygen and grease barrier failure in the thin coatings was primarily due to local defects rather than average thickness. The observed differences in pinhole density can explain the measured barrier performance. Achieving effective barrier coatings at elevated machine speeds on rough paperboard substrates, in the absence of a precoating layer, presents considerable challenges. In the present study, the rates of oxygen transmission summarised in Table 7 and Figures 3–5 are slower than reported elsewhere. Olsson et al. [74] reported OTR values that exceeded 1000 cm 3 m − 2 day − 1 at a total coat weight of 9.1 g m − 2 for starch/bentonite/PEG coatings applied at 500 m min − 1 on liquid packaging board. Changing the substrate to a smooth and dense greaseproof paper resulted in a minimum measured OTR of 74 cm 3 m − 2 day − 1 [74], indicating the benefits of smooth substrates when applying aqueous barrier coatings at high machine speeds. It is anticipated that conducting analogous multiple coating trials on a smooth and mineral precoated paperboard would yield substantially lower oxygen transmission rates. The oxygen transmission measured for sample A6 was higher than anticipated based on the oxygen permeability of laboratory-cast montmorillonite/starch films [68]. This discrepancy may stem from local variations in coating thickness, even though Figure 2 and Table 5 indicate a pronounced contour coating. The comparatively low coat weight recorded for sample A6 (5.1 g m − 2 ) increases the likelihood that certain regions received insufficient coating, thereby creating local weaknesses in the barrier layer. Furthermore, it is conceivable that minor defects in the coating layers may become increasingly influential after the principal voids between cellulose fibres were sealed after the first two layers.
https://doi.org/10.3390/coatings16030299
Made with FlippingBook Online newsletter maker