Coatings 2026 , 16 , 299
20of 25
Table 6 revealed that compression of the substrate is needed to fill the surface irregu- larities between fibre flocs, leading to a uniform coating. The characteristics of the resilient metering tip used in the present study are also expected to contribute to coating unifor- mity [90]. In addition to the material properties, the shape and angle of the resilient tip influence the degree of compression, in line with the force balance outlined by Renvall and Kuni [33]. The use of an integrated applicator/metering of the short-dwell type and the use of a base paperboard with a low Cobb value further helped to ensure a sufficient wet volume beneath the metering blade. Overall, the findings indicate that coating uniformity is influenced not only by the dryers and machine speed, but also by the design of the coater. Previous studies have demonstrated that the coating uniformity becomes highly dependent on the coating technique within the wavelength range 1–8 mm [91]. In a study address- ing multilayer PVOH barrier coatings, Christophliemk et al. [47] proposed that excessive compression during metering may induce small-scale defects, typically a few micrometres in size—resulting from surface compression followed by relaxation. In the present study, a resilient polymer metering tip was selected to mitigate such defects. Furthermore, the optical resolution of the Michelson objective employed in the present study was inadequate for detecting minute surface defects caused by compression and relaxation. Optimisation of coating parameters such as machine speed, blade tip angle and coater pressure was beyond the scope of the present study, as these variables remained constant during all multilayer trials. However, further optimisation of the coating parameters could have resulted in additional reductions in oxygen permeability. Although the AOIR and OTR values presented in Table 7 do not fulfil the require- ments for effective oxygen gas barrier performance, all multilayer-coated samples without pinholes exhibited outstanding grease resistance. These findings suggest that the thin multilayer coating approach can be successfully applied in paperboard manufacturing to achieve superior grease resistance, thereby obviating the necessity for mineral precoating. 4.4. Food Contact Starch is a hydrophilic material and starch films may slowly dissolve in contact with water. This must be considered when starch films and coatings are used in packaging applications [92]. According to Commission Regulation (EU) No 10/2011, plastic materials and articles must not release more than 10 mg of constituents per dm 2 of contact surface into food simulants. Crosslinking of starch has been proposed as an effective strategy to comply with regulatory requirements concerning overall migration limits, while simultaneously reducing the solubility of starch-based films in aqueous environments [73,74]. 5. Conclusions The present study focused on traditional coating techniques, i.e., applying excess coating colour and then metering to achieve the desired coat weight. The coater was equipped with a resilient metering tip, and the design was aimed to minimise the dwell time between application and metering, thereby reducing sorption of the coating colour or its aqueous phase into the substrate. Thus, the conclusions strictly apply to such techniques. Since the present study addresses drying effects, most findings related to drying settings are likely applicable to other wet coating techniques for paper or paperboard, as well as other water-borne coating formulations. The most important findings were as follows: • To fully realise the benefits of multilayer technology, it is essential to implement an optimised drying strategy. • An excessive power setting in the IR dryer led to a higher incidence of pinholes and increased oxygen penetration in the multilayer-coated samples. Further elevation
https://doi.org/10.3390/coatings16030299
Made with FlippingBook Online newsletter maker