J Renew Mater. 2025
7
3.2 Mechanical Properties 3.2.1 Density
EPW1 biocomposites, composed solely of egg packaging waste, exhibited significantly higher density compared to EPW2 and EPW3 combinations containing hemp and sawdust co-substrates, respectively (Table 2). The density of the composites was closely linked to the substrate composition and particle size distribution. EPW1, comprising 60% coarse particles ( > 10 mm), yielded the densest composite (0.24 g ⋅ cm − 3 ). In contrast, EPW2, incorporating hemp shives with a porous, loose structure, resulted in the lowest density (0.15 g ⋅ cm − 3 ). EPW3 composites, combining fine sawdust and coarse EPW particles, showed intermediate density (0.19 g ⋅ cm − 3 ). These results align with reported density ranges for mycelium-based composites (0.06–0.30 g ⋅ cm − 3 ), where agricultural by-product fillers such as straw yield lower densities than forestry residues like sawdust [45]. Similarly, Teeraphantuvat et al. [46] demonstrated that MB density increases with higher paper waste content, with the highest values (0.32 g ⋅ cm − 3 ) observed in sawdust-based composites containing 40% paper waste. Table 2: Mechanical properties of EPW mycelium biocomposites. EPW: egg packaging waste; Compositions 1–3 correspond to different substrate formulations. Values are presented as mean ± SD Composition of biocomposite Density (g ⋅ cm − 3 ) Compressive strength (MPa) Compressive modulusof elasticity (MPa) Flexural strength (MPa) Flexural modulusof elasticity (MPa)
EPW1 EPW2 EPW3
0.24 ± 0.01 0.18 ± 0.06 0.15 ± 0.00 0.32 ± 0.01 0.19 ± 0.00 0.22 ± 0.07
2.90 ± 1.74 8.11 ± 0.83 4.37 ± 1.99
0.95 ± 0.26 25.96 ± 6.23
0.63 ± 0.05 0.89 ± 0.08
18.47 ± 6.85 18.60 ± 1.66
3.2.2 Compressive Strength Compressive strength of EPW mycelium biocomposites ranged from 0.18 to 0.32 MPa, while the compressive modulus of elasticity varied between 2.90 and 8.11 MPa (Table 2). EPW2 samples containing hemp exhibited significantly higher compressive strength ( p < 0.05) compared to EPW1 and EPW3. Although cellulose fibers possess high strength and stiffness [47], the higher density and predominance of coarse particles in EPW1 likely hindered fungal colonization, reducing compressive strength. Conversely, the porous structure introduced by hemp shives in EPW2 facilitated improved fungal growth, enhancing mechanical performance. Similar trends were observed by Teeraphantuvat et al. [46], who reported decreased com- pressive strength with 40% paper waste addition in sawdust composites, while a 30% paper waste addition to corn husk composites improved strength. Elsacker et al. [48] demonstrated that MB with dense fungal colonization exhibit higher compressive stiffness, highlighting the significant influence of fungal morphology and substrate interaction on composite properties. Their study reported the highest compressive stiffness (0.51 MPa) in composites with hemp additions, whereas wood-based samples showed the lowest stiffness (0.14 MPa). In the current study, the lower density of hemp-containing composites can be attributed to the inherently low density of hemp particles (0.068 g ⋅ cm − 3 ) rather than overall composite density. Fungal growth in the void spaces of hemp composites likely created air pockets supporting sustained hyphal development. Consequently, dense mycelium networks contributed to improved compressive properties, as observed in EPW2 samples.
Made with FlippingBook Online newsletter maker